Does anyone see where on this MTR it says normalized? I can’t find it, I see the Specification but it says MT - usually they just have N for normalized.
So if you go into ASME Section II Part A-2 and look up SA-516, it will tell you that plates 1.5" and under are supplied in the as-rolled condition, but they may be ordered Normalized if required by the purchaser. For general requirements of plate steel, including marking and identification, you have to go to SA-20 (General Requirements for Steelmaking). Paragraph 13.1.2 of SA-20 says " Plates that are required to be heat treated, and have been so heat treated, shall be marked, by the party that performed the heat treatment, with the letters “MT” (denoting material treated) following the required ASTM designation mark.
Adding to the SA-516 point above: if the PO called for normalized plate, the MTR has to show it. Look in the heat treatment or condition field, the supplementary requirements, or notes like "Normalized" or "N" next to the grade. If none of that is there, don't assume it from the tensile or yield numbers. As-rolled and normalized plate can both meet the same mechanical minimums. Write it up as a nonconformance or hold the material, and ask the supplier or mill for a corrected MTR or a heat treatment certificate tied to that heat number. If they can't give you one, it's an engineering or purchasing decision, not an inspection call.
2
u/Whole-Worldliness260 6d ago
Was it supposed to be normalized?
6
u/eyarzab 6d ago
So if you go into ASME Section II Part A-2 and look up SA-516, it will tell you that plates 1.5" and under are supplied in the as-rolled condition, but they may be ordered Normalized if required by the purchaser. For general requirements of plate steel, including marking and identification, you have to go to SA-20 (General Requirements for Steelmaking). Paragraph 13.1.2 of SA-20 says " Plates that are required to be heat treated, and have been so heat treated, shall be marked, by the party that performed the heat treatment, with the letters “MT” (denoting material treated) following the required ASTM designation mark.
1
u/LHTX27 6d ago
Thanks
1
u/Admirable_Cell_2933 3d ago
Should be able to tell by the mechanical properties