r/electroplating • • 16d ago

What changed? Someone please help!!!

So my gold plating was going along really well. Then this morning I topped up my 18ct bright gold soloution from goldpatingservices and woods nickel strike both with small amounts of distilled water, just to get them back to the 1 litre mark ( as directed by goldplatingservices ) and now when I have tried to plate, the gold is adhering in patches and the top seems the be playing better than the lower half.

What have I done? I asked AI ( I know they are far from a reputable source of information when needing technical help) but that's all I have to work with, and it decided that the water has not been incorporated properly yet and after thorough stirring in it will work properly again.

I don't trust it, that's why I am here asking for help and ideas.

I have made another woods nickel strike soloution, because it seemed that it might have been the woods where the problem is because the gold is affixing in patches, but that hasn't changed anything. I am now in the process of polishing it all back to the stainless and starting again. I hope this helps

10 Upvotes

22 comments sorted by

3

u/tennepenne1 16d ago

Maybe poor conductivity, not sure responding to bump this so someone else sees

3

u/1984isnoww 16d ago

If you're plating stainless steel, you should be using TriVal 24k for prepatory process. If you plate PVD use Acid dip.

As always obsessively clean before you plate.

Dishsoap scrub with brush>ultrasonic>electrocleaner>TriVal>18k

De-Ionizied water rinses between each process and have dry microfiber towels on hand to pat dry after rinse (if you have compressed air or steam clean this is better)

Also I'm not sure what equipment you're using but make sure you're using good stainless steel wire and look at my history to see how I wire up my parts for plating.

2

u/Primary-Dog4923 15d ago

Thanks for giving me some pictures to see how to wire up correctly

1

u/chucknwatches 15d ago

Superb answer 🫡

2

u/permaculture_chemist 16d ago

Just to be sure, but you played the nickel first, rinsed, and then went to gold?

How much time between the nickel and gold? Too much time will cause the nickel to passivate and the gold won’t adhere.
What type of rinse between the nickel and gold? High-purity water can passivate nickel and cause subsequent plating issues like this.

1

u/Primary-Dog4923 15d ago

Yeah I did as you said in the top line. The only time between was the amount of time it took to take the clip off the nickel anode and connect it to the platinized titanium in the gold bath. Between the baths I do two distilled water rinses. But like I said this set up has worked perfectly for a couple of weeks and it wasn't until I topped up the baths with distilled water up to the 1 litre mark (about 50mls) that this problem started

1

u/spiderman3098 15d ago

May have ruined the electrical property by diluting the solution

1

u/Primary-Dog4923 15d ago

The resources page on the website says to top up with distilled water as it evaporates

1

u/spiderman3098 14d ago

Yea but if thats the only thing that changed between the process id assume that is the problem

1

u/permaculture_chemist 14d ago

Try to “sour” the rinses with a bit of the next solution. We find that 1% of the next bath (the gold in this case) in the rinses help cut the tendency of the pure water from passivating the nickel layer.

1

u/Ok_Deer_7058 11d ago

After the nickelbath, swith the polarity for a minute. It makes your plating somewhat mat but with some extra polishing your next plating will improve.

1

u/CaffeineConduction 16d ago

What's your pre treatment process on both cases?

1

u/Primary-Dog4923 16d ago

I did them both in the same time. I ultra sonic clean 50⁰c 15 mins, then electro clean 4amps cc mode 45⁰c 45 second cycles until wetted then woods nickel strike 4amps cc room temp 45 sec and then finally 18ct bright gold soloution at 40⁰c agitated . 56amps upto 7 mins. Everyday this week it has worked fine and then I topped up the woods nickel and gold soloution this morning before starting and that was the result

1

u/CaffeineConduction 16d ago

How was the voltage during the process?

Do you have the possibility to run a hull cell?

1

u/Primary-Dog4923 16d ago

I am pretty new to this gold plating stuff. Sorry if I sound stupid but what is a hull cell? I don't know where to find the information that I need and have just been researching by myself and picking things up along the way. I still feel like I am reaching in the dark with most things

1

u/CaffeineConduction 15d ago

It's a test to measure the electrolytes behavior in different current density areas Google it.

But it's probably too much to ask for considering your current state of tech.

1

u/Primary-Dog4923 16d ago

There is three settings on the front of the rectifier. 16v/5a, 27v/3a and 36v/2a. The gold plating supplier that I brought it off said to just leave it on the 16v/5a setting and set the volts to 16.5 and then have it on CC mode and just adjust the amps. I think I accidentally switched it to the 27v/3a setting this morning sometime because I had big rubber chemical resistant gloves on. Would this have made a big difference?

1

u/CaffeineConduction 15d ago

Yes it will be a problem. As gold is coming from a gold complex, high current density will disturb the complexometric process

1

u/CaffeineConduction 16d ago

Giving parallel a few assumptions and a few other questions:

Did the Woods Nickel Apply correct, or has it already some spots?

If it already has problems in the woods, it could be that after diluting your Chloride Content is too low and can't therefore plate good on the Steel.

Also I always recommend to activate the part anodic before going into the Nickel. It prevents most problems and doesn't hurt.

If the Problems only occur from the Gold:

Did you rinse enough before going from the Acid Nickel to the alkaline Gold?

It's always best to rinse, pickle (not the right translation but I don't know the right one in English) in a low % sulfuric acid solution, and rinse again before going into the Gold.

Did you rinse hot after the Gold? Always rinse hot. Like very hot. 70°C or more. Some alkaline and additives in the Gold Elektrolyte can Stick to the surface and create alterations of the Gold layer, especially if it's thin, and cause problems.

Gotta go back to work, will have look later and think of other reasons that come to my mind.

1

u/Primary-Dog4923 16d ago

I'm not sure if the nickel is applying correctly or not. How could I tell? I am not sure if it is a problem with the nickel strike or the gold

1

u/CaffeineConduction 15d ago

Nickel Looks more yellowish compared to the steel but not as yellow as the gold