r/fusedglass • • 21d ago

Help retaining rectangular shapes when full-fusing Bullseye COE 90 glass

I'm relatively new to glass fusing and have been experimenting with my firing schedules. I'm hoping someone with more experience can help me figure out how to retain the original rectangular shape of my panels while still achieving a smooth, full fuse.

I'm making glass photo panels, so keeping the dimensions and shape relatively consistent is important.

My setup:

- Bullseye COE 90 glass

- Orton AutoFire 3000 controller

- Two layers of 3 mm glass (approximately 6 mm total)

- Various panel sizes, including 4×6, 5×7, and 8×10 inches

- Firing on kiln shelf paper

My original full-fuse schedule (°F):

Segment| Rate| Target| Hold

1| 300°F/hr| 1225°F| 45 min

2| 600°F/hr| 1480°F| 10 min

3| AFAP| 900°F| 60 min

4| 150°F/hr| 700°F| 0 min

I was getting a nice, smooth full fuse, but the glass was spreading and rounding considerably. The corners were becoming very rounded, and the panels were losing their original rectangular shape.

What I changed:

I decided to try reducing the peak temperature from 1480°F to 1470°F while keeping the 10-minute hold and the rest of the schedule the same.

My revised schedule (°F):

Segment| Rate| Target| Hold

1| 300°F/hr| 1225°F| 45 min

2| 600°F/hr| 1470°F| 10 min

3| AFAP| 900°F| 60 min

4| 150°F/hr| 700°F| 0 min

What happened:

I've attached photos comparing the results from the different schedules.

The green/yellow panel shows that reducing the peak temperature helped somewhat. It retained more of its original rectangular shape compared with the previous firing.

However, I'm still getting significant rounding of the corners, uneven edges, and some distortion along the sides. The glass seems to pull inward in some areas and spread outward in others, rather than maintaining relatively straight edges.

The reddish panel also illustrates the kind of rounding and shape distortion I'm trying to avoid.

I've also been working through some bubbling issues, but I think I've largely figured those out. Right now, my main concern is shape retention, rather than bubbles.

My questions:

  1. Would you recommend reducing the peak temperature further, perhaps to 1460°F, or shortening the 10-minute hold instead?
  2. Is there a point where lowering the temperature will prevent the two layers from fully fusing together?
  3. Is this amount of rounding and distortion simply unavoidable when full-fusing two layers of 3 mm glass?
  4. Would changing the firing schedule help maintain straighter edges, or should I be looking at other techniques?

I'm not expecting perfectly sharp corners, but I'd love to get closer to the original rectangular shape without sacrificing the smooth, fully fused surface.

Any advice would be appreciated! I'm trying to understand the relationship between temperature, hold time, and shape retention rather than just experimenting randomly.

5 Upvotes

16 comments sorted by

13

u/Claycorp 21d ago
  1. You are going very hot to retain the actual shape. Glass does not want to be square, it wants to be round and will heat from the edges in. You want to reduce total temperature if you have no reason to go that hot.
  2. What do you mean by "fully fusing together" because even a tack fuse will attach the two parts together. Glass is special in how it works there's no solid -> liquid change. Once it gets to a certain temp it will stick to other glass without moving really at all. Going hotter and hotter only makes it move around more. Holding the lower temp longer also allows it to bond better in the case of dealing with air pockets.
  3. Pretty much with how hot you are going. Glass when moving has surface tension just like anything else liquid. That's why all the white powder is on the corners and pulled up. the surface tension has pulled the non-round parts in while it's trying to make something round. It also almost looks like your kiln isn't level as the left of both parts look thicker and the glass seems pulled in that direction.
  4. Reducing working temp keeps more shape. Kiln work is all about working temperature and time. More temperature = more movement. More time = more movement. You want as little of both as you can get away with.

2

u/dontstopbelieving 20d ago

Hi there! Thanks for taking the time to respond.

So, I want it to essentially look like one piece of glass. I don't want to see the seam (like you would with a tack fuse). I want it as smooth as possible while retaining as much of the shape as I can. I don't mind rounded corners at all, but I want the pieces to maintain a lot more of their shape and not countour in. Would you have a recommended schedule for that kind of output?

5

u/Claycorp 20d ago
  1. Reduce your starting hold temperature so it's just below the sticky state, it won't move but will still be safe here. 1175F. This gives you more runway to get the kiln to working temp without the glass moving too much as it's heating
  2. AFAP to your working temp which we will reduce to 1440F, hold for 5-10 minutes. You pick where to start. if 5 is still way too much reduce step 1 by another 50-75 degrees. If 5 is just a bit too much, try 3. If the number you picked wasn't enough just keep adding time.
  3. Keep the rest the same.

Half of kiln work is just workin on vibes because every kiln fires differently, what's in the kiln changes the outcome, the phases of the moon, what the kiln is made of... Everything. Just gotta keep trying to change parameters till you get something you like while taking notes the whole time. Though it's usually better to change fewer things at once than it is to go all out modifying many steps but because you are so far off of what you want multiple steps is a better way to find a closer point to what you want.

1

u/dontstopbelieving 18d ago

Thank you so much! I reduced peak temp to 1440F for ten minutes and they came out perfectly!!

2

u/Claycorp 18d ago

Yay! Now keep notes of that!

2

u/laurenfosterskittens 18d ago

lmao the phases of the moon i stg

2

u/very-jaded 21d ago

Even 1460 is still too hot, giving you a full fuse where the glass turns fully liquid. It sounds like you want either a contour fuse, which would give you rounded edges while retaining the original shape, or a tack fuse which will stick the glass together but retain the exact original shape, only with polished edges.

For a tack fuse, set the process temperature to 1350 and hold for only 1 minute before dropping down to your anneal.

For a contour fuse, set the process temperature to 1420 with a 14 minute hold.

Try the tack fuse first, and if you don't like the results, re-fire it to a contour fuse.

2

u/very-jaded 21d ago

I've been looking at your other scheduled steps. I'd go AFAP from the pre-heat soak to the process temperature (your step 2).

When you're done with the pre-heat soak the glass is soft and not at risk of cracking, and you want to spend as little time as possible getting to and from your process temperature so that you don't get any unwanted side effects.

3

u/dontstopbelieving 20d ago

Ok, I will try the contour fuse. That might be what I am going for, although I am hoping the surface is quite smooth!

4

u/Plane_Entertainer_88 20d ago

Been fusing for 25 years; originally taught by Bullseye’s staff when they invited potential instructors.

Ditch the paper; expensive and unnecessary. Learn to apply kiln wash and spend your money on glass.

The goal is to achieve the results you want with the glass being subjected to as little heat as possible. In my smaller kilns, I would fire your piece like this:

300° to 1150° hold 0

50° to 1250°, hold 45 (this is your bubble squeeze)

400° to 1400°, hold 10

Then anneal as you were.

1

u/nemaihne 20d ago

Everyone else has answered this from the heat side, and better quite well.
So I'm going to mention another angle. Some of this is also a question of thickness. Glass wants to be circular. It is also particular about thickness of the layers. You get the least deformation at 6mm. More that that and the outsides are likely to bow a bit in a fuse, less and the sides will pull in. So it's fairly obvious from both pieces that you are a bit less than 6mm.

1

u/dontstopbelieving 20d ago

Not sure why that is as I am using 2 pieces that are 3mm thick!

3

u/Zealousideal_Sir_975 20d ago edited 20d ago

I think we are seeing two issues combined. As one person mentioned, your kiln shelf does not look like it's truly level. With such a hot and long fire, the glass wants to flow to balance out the need for even surface tension and a level liquid surface. As gravity draws glass away from the right edge and it gets thinner, the surface tension is drawing in that edge, lifting the corner glass to flow toward center and dog boning the right edge to seek 6mm. The left side edge and corners are flowing left and outward due to gravity generally moving the glass leftward so that side is rounding out more. Too long, too hot causes too much glacial flow. Shorter times and cooler kiln means the glass remains closer to the starting shape.

At tack, the corners are nearly square and the edges stay nearly straight and vertical, just smoothed over. The top surface still retains much of its rolled texture.

At contour the edges look more rounded off and the corners get a quarter inch radius. The top surface starts to lose its texture from being rolled but still has some shape like very gently rippled pool water.

At full fuse, the liquid's top surface will find its level and all texture (absent coatings/impurities) will be lost.

If your goal is a mirror smooth top surface with sharp rectangular corners, those are contradictory outcomes. You can get there a couple ways. One is to go full fuse with a larger piece of glass to get your desired top surface, then cut off the uneven rounded edges to get back to rectangular. (Score and break or tile saw and/or lap wheel.) Firepolish the cuts (either the flat glass or while slumping to a shape.)

The other ... If precision corners are not that important but straight edges are, do the full fuse in a dam mold that will give you your straight edges and corners without concern for going longer or hotter (as long as it's level). These molds are generally known in the industry as Patty Gray molds after the designer that came up with the just-right shape. As long as there is enough glass in the mold to result in a 6mm thick slab, the edges are straight, the corners have under a quarter-inch radius and the top is mirror flat after a full fuse firing that has a long enough bubble squeeze to outgass any glues that were used.

Two pieces of 3mm glass cut to fit a Patty Gray mold can be light on glass and pull away from the dam walls. This is because 3mm rolled glass is not consistently 3mm thick. The surface texture comes from slightly less glass between the rollers. Also, cut glass does not precisely fill the lid to the edge. So, some artists will lay in the first sheet of glass into the bottom of the prepared mold, then sprinkle clear glass powder to fill in the valleys of the surface texture and a bit more of the top sheet, then lay on the top sheet. To solve cutting the glass smaller than the dam, fill the edges with clear fine frit until at least as high as the top of the top sheet (or a bit more). An advantage of the powder between the sheets is a change in the appearance of the inevitable bubbles that remain. Instead of fewer larger champagne bubbles, you get finer ones that create more of a misty look.

For absolute certainty that you have the minimum amount of glass to not dogbone way from the walls of the dam, each mold has a weight of glass in grams that is the minimum for proper shape. You weigh the empty mold, then weigh the mold with glass sheets in it and keep adding frit until the ideal target is reached or exceeded. This is overkill for a couple pieces of sheet glass, but is great when piling up your scrap glass to make a new, very-rectangular panel without the need for coldworking.

Finally, you can conform a hand-made dam to the dimensions of your glass. Get refractory fiber paper and cut strips for the four edges and use kiln posts lying on their sides to hold the paper vertically against the edges of the glass sheets. The glass will be shaped by the fiber paper to remain straight and not flow. This is overkill for two sheets, but works great for effects like "optics" where you intend to flow the center glass while remaining rectangular.

1

u/Gordonica 20d ago

you have to damn them

1

u/Gordonica 20d ago

you have to dam them