I think this is not only my first post in this sub, but also my first ever Reddit post. It'll be a long one, so bear with me.
Tl;dr: I had a terrible first layer when printing ASA. I fixed the problem, by introducing a Z-offset of 40 µm. I believe it is caused by the temperature delta between probing the bed at 150 degrees and printing at 260.
Last week, I got my very first 3D-printer, a Prusa Core One L+. I love that thing! It's truly addictive and I was working with it non-stop. I started printing my first benchies and the robo alpaca in Prusament PLA Galaxy Black (pics attached) and then quickly switched to PETG for some functional prints, like the nozzle change tool.
Next on my list was ASA and I already had some project ideas: I wanted to print some parts to mod the Buddy3D cam and a 1:48 model of a fighter jet. The first tries were okay, but not great. The surfaces were uneven and especially the first layer was a desaster.
I am using Light Grey ASA from 3DJake and applied the Prusament ASA default profile. 3DJake gives an ideal temperature of 230 degrees +-20, while the Prusa profile uses 260 degrees. Being new to ASA, I thought that the temperature maybe was too high -> I decided to print a temp tower. To me, it looked like the tower confirmed 260 degrees as good.
The first layers still were terrible. However, I observed that the perimeter layed down perfectly. Only the infill of the first layer looked disgusting. Idea: The perimeter is printed slower than the infill, maybe my speed is to high. -> I reduced the print speed of the first layer infill, to match the perimeter speed.
It still sucked. The first layer looked very soft and gloopy. New idea: maybe the bed is too hot? -> I played with the bed temperature. Everything between 90 and 110 degrees.
You guessed it: it still didn't fix the issue. So I showed it to some friends, who have some years of experience with 3D printing. Their idea: over extrusion. Consequently, I downloaded Orca slicer, for the flow ratio calibration. While printing the tabs, I had a close eye on the first layer: Reducing the flow ratio seemed to help, but at a ratio of 0.85(!) I was still seeing the issue. All the while, the printed tabs showed under(!) extrusion on the top layer. I also printed one of the thin walled boxes, which confirmed that I actually should be printing with *more* material, as the walls were thinner than they should.
Obviously, a larger flow ratio made the problems even worse. So I kept on digging. I recalibrated my Z-axis, I checked wether the nozzle is mounted properly, I recalibrated every feature on the printer, including the belts and extruder. I also dried the filament and stored it in the Prusa dry box during printing. All to no avail. After some more digging, I came across this old Git: https://github.com/prusa3d/Prusa-Firmware-Buddy/issues/4254
Users had a problem with wavy first layers, that looked a bit like mine, just less scrapy. They reported, increasing the z-offset by 40 µm fixed the issue.
On the Core One L+, this really should not be a thing. After all, the printer is probing the bed, to make sure that it is really level. But then I looked at the exact probing procedure: My printer is heating the nozzle to 150 degrees for probing. However, I am printing ASA at 260 degrees. Did this delta of 110 degrees mess with my tolerances?
The nozzle is screwed into the hot end and sticks out a bit. However, the hot end by itself, is mounted to the nozzle, which is clamped near the heat break in the extruder. The bit that is sticking out of the extruder is ~23 mm long, of which a small part is steel, while ~20 mm are brass. Brass has a thermal expansion coefficient α of ~ 18.5 x 10-6. Thermal expansion of a material is given by
ΔL = α * L * ΔT
So, for the piece of brass of 20 mm lenght we find an expansion in lenght of... 40.7 µm! Coincidence?
To test the hypothesis, I printed a single layer using this model from printables and manually increased the z-offset in steps of 10 µm. If this all is working out, I indeed should see that my problem goes away at a Z-offset of ~40 µm.
Heureka! A Z-offset of 40 µm and the printer layed down a near perfect layer (see pictures)!
I lost days of sleep over this and burned through quite some filament, so I felt like sharing this with you fine people. Maybe someone finds it helpful. Maybe someone at Prusa also wants to have a look at a thermal expansion compensation in the firmware ( u/nomadsgalaxy u/Tommy_Prusa3D ?).